PipingDesigners Community

A place for piping designers, engineers and industry professionals to ask questions, share experience, discuss technical topics and connect with other professionals.

Browse the discussions below or start a new topic. Please keep discussions practical, professional and relevant to the piping and engineering community.

L flanges are limit...
 
Notifications
Clear all

L flanges are limited (per ASME B16.5) to 425 deg C, while 304 flanges go up 1500 per ASME B16.5. If you have dual…

12 Posts
3 Users
0 Reactions
77 Views
(@hvn83)
Eminent Member
Joined: 16 years ago
Posts: 12
Topic starter   [#343]

Hi all,

I'm fairly new to this board, this will be my first post.
The question I'd like to ask deals with dual certified 304. I've already google-ed this topic a lot but I cant find a satisfying answer to my question.

Right now, the company I work for (we work in e.g. the (petro-)chemical industry) is making a new pipe spec for 304 material.
We didn't have any for 304 spec before, so I thought of, while making the new 304 spec, to use dual certified 304, since it's good available as such, and has almost the same parallels as 316/316L (for which we already had a spec).

Now, the one thing bothering me is that 304L flanges are limited (per ASME B16.5) to 425 deg C, while 304 flanges go up 1500 per ASME B16.5.
If you have dual certified 304/304L flanges, can you then 'just' use such dual certified flanges up to and above 425 deg C?

The second question (not that important but still interesting); what would you have to do if you want to use 304/304L piping systems beyond 1000F (~538 deg C)?
What values for stresses do you then use, how do you do the calculations?



   
Quote
(@hvn83)
Eminent Member
Joined: 16 years ago
Posts: 12
Topic starter  

Hi shrivallabha,

Thank you kindly for your answer.
I already noticed that thread, but it doesn't mention anything about the temperature range 304/304L may operate in, regarding the limits of 304L flanges.
Hence my question is still open.



   
ReplyQuote
(@shrivallabha)
Estimable Member
Joined: 17 years ago
Posts: 134
 

The post #4 by JamesKelly mentions Temperature suitability

Almost all "304" plate is dual certified. It may be 0.03 max carbon stuff dual certified 304L/304. This, meanins it has decent corrosion resistance as-welded and the tensile & yield properties of 304, at least near room temperature.1150F is in the creep range, for which you need dual certified 304/304H. This has a minimum of 0.04% carbon for strength, plus I think both grain size and minimum annealing temperatures. It is widely available.Dual certification is the common practice. The mill does not want to melt two or three different chemistries, i.e. 304L, 304 and 304H so they make two different chemistries do the work of these three. It is the magic of precise chemistry control by refining the melt in an Argon-Oxygen Decarburization vessel, where a little nitrogen brings up the yield strength of 304L to the requirements of 304. Great for room temperature but the dual-certified "L"grade is not usually considered strong enough for use in the creep-limited range.Clear as mud?

If you go by this post then you should avoid using Dual Certified Steel (L) at higher temperatures and should go for the other Dual Certified Steel(H).

See if this is of any help!



   
ReplyQuote
(@hvn83)
Eminent Member
Joined: 16 years ago
Posts: 12
Topic starter  

The post #4 by JamesKelly mentions Temperature suitability

Almost all "304" plate is dual certified. It may be 0.03 max carbon stuff dual certified 304L/304. This, meanins it has decent corrosion resistance as-welded and the tensile & yield properties of 304, at least near room temperature.1150F is in the creep range, for which you need dual certified 304/304H. This has a minimum of 0.04% carbon for strength, plus I think both grain size and minimum annealing temperatures. It is widely available.Dual certification is the common practice. The mill does not want to melt two or three different chemistries, i.e. 304L, 304 and 304H so they make two different chemistries do the work of these three. It is the magic of precise chemistry control by refining the melt in an Argon-Oxygen Decarburization vessel, where a little nitrogen brings up the yield strength of 304L to the requirements of 304. Great for room temperature but the dual-certified "L"grade is not usually considered strong enough for use in the creep-limited range.Clear as mud?

If you go by this post then you should avoid using Dual Certified Steel (L) at higher temperatures and should go for the other Dual Certified Steel(H).

See if this is of any help!

Thanks again for the explanation, but it still ist an answer to my question (I believe).
I'm talking specifically about the 0 deg C - 425 deg C (~ 842 F) temperature range, which is below the range mentioned in your last post.
Second, I'm dealing with flanges, not with plates.

See the corresponding ASTM and especially the ASME B16.5 design notes; then you'll understand where my question comes from.

Briefly; 304L flanges may only operate up to 425 deg C (per ASME B16.5).
So, may 304/304L flanges (say 150 lbs) operate up to 538 deg C then?
Why or why not?



   
ReplyQuote
(@hvn83)
Eminent Member
Joined: 16 years ago
Posts: 12
Topic starter  

The post #4 by JamesKelly mentions Temperature suitability

Almost all "304" plate is dual certified. It may be 0.03 max carbon stuff dual certified 304L/304. This, meanins it has decent corrosion resistance as-welded and the tensile & yield properties of 304, at least near room temperature.1150F is in the creep range, for which you need dual certified 304/304H. This has a minimum of 0.04% carbon for strength, plus I think both grain size and minimum annealing temperatures. It is widely available.Dual certification is the common practice. The mill does not want to melt two or three different chemistries, i.e. 304L, 304 and 304H so they make two different chemistries do the work of these three. It is the magic of precise chemistry control by refining the melt in an Argon-Oxygen Decarburization vessel, where a little nitrogen brings up the yield strength of 304L to the requirements of 304. Great for room temperature but the dual-certified "L"grade is not usually considered strong enough for use in the creep-limited range.Clear as mud?

If you go by this post then you should avoid using Dual Certified Steel (L) at higher temperatures and should go for the other Dual Certified Steel(H).

See if this is of any help!

Thanks again for the explanation, but it still ist an answer to my question (I believe).
I'm talking specifically about the 0 deg C - 425 deg C (~ 842 F) temperature range, which is below the range mentioned in your last post.
Second, I'm dealing with flanges, not with plates.

See the corresponding ASTM and especially the ASME B16.5 design notes; then you'll understand where my question comes from.

[b]Briefly; 304L flanges may only operate up to 425 deg C (per ASME B16.5).
So, may 304/304L flanges (say 150 lbs) operate up to 538 deg C then?
Why or why not?[/b]

Bump, anyone?



   
ReplyQuote
(@karthi090287)
New Member
Joined: 16 years ago
Posts: 3
 

Hi all,
im new to this forum,
i have 1 question ,due to lower carbon content in the ss304L(0.03%),is it restricted to use below 425 deg celcius or any other reason is behid this??
Can any one explain me wat is the Temperature range for SS304L ,SS304 ,SS304H???



   
ReplyQuote
(@hvn83)
Eminent Member
Joined: 16 years ago
Posts: 12
Topic starter  

Hi all,
im new to this forum,
i have 1 question ,due to lower carbon content in the ss304L(0.03%),is it restricted to use below 425 deg celcius or any other reason is behid this??
Can any one explain me wat is the Temperature range for SS304L ,SS304 ,SS304H???

I think the reason behind this is the carbon content indeed.
I'm not quite sure, but I believe (please correct me if im wrong) that it has something to do with the resistance to high temperatures @ low carbon containing stainless steels.

Tip: just Google 'dual certified 304' and look for a thread going @ engtips.com (I think its the first Google result)



   
ReplyQuote
(@karthi090287)
New Member
Joined: 16 years ago
Posts: 3
 

hi HVN83,
i got ur question,dual certified 304/304L is used up to 537 degree celcius,because the carbon of this steel has the same percentage as normal ss304, if u refer ASME B16.5 ss304 materail and the temp range for the same is given,u will get better understanding



   
ReplyQuote
(@hvn83)
Eminent Member
Joined: 16 years ago
Posts: 12
Topic starter  

I'm sorry but so far no one has really understood, nor answered, my question.
To put it in perspective again, here comes a new formulation of the same question:

If you use dual certified have 304/304L ASME B16.5 flanges, what is/are the max. temperature (limits) these flanges may be used to, and WHY?
B16.5 namely does not address any reasons why 304L flanges are limited to 425 deg C.
It only says 304 flanges may be used to 816 deg C, and 304L flanges up to 425 deg C.
Thus, what temperature limit should be used now for dual certified 304/304L?

PS: if Im making a mistake, i.e. my question has been answered, Im sorry if I understood the respective reply wrong. Just let me know where the answer is mentioned.



   
ReplyQuote
(@shrivallabha)
Estimable Member
Joined: 17 years ago
Posts: 134
 

I tried to search as well but it all seemed to be going nowhere. Here is some explanation (and not all). We'll try to understand in step by step manner.

First, what defines the grade 304L, 304 and 304H?
The chemical composition i.e. Carbon content prominently. There is a grade comparison table on AZOM.com. If you have close look then 304L satisfies all criteria of 304 (chemical composition wise). This, probably, is the reason why the material is claimed in dual grade as it will reduce inventory.

What is the effect of Carbon on steel?
SS as it is also known as Austenitic steel allows more carbon solubility than many other steel grades. As you go on increasing carbon content it becomes harder and stronger (but less ductile). This explains as why the carbon content is increased for higher temperature ranges. The same is noted by ASME in ASME B 16.5, Table 2-2.1, Note(1).

What temperature range shall be used for dual certified steel?
This part still remains little gray. I tried to find some references which could pin it down. However, following excerpts from ASME might be useful.

At low or high temperatures, the designing person shall consider a possibility of leakage at joints due to forces and moments developed into the connected piping. When such joints are operating at creep range, the bolt loads will relax due to expansion. Such decreased bolt loads diminish the capacity to effectively sustain loads without leakage. These are]
So it indicates it is rather joint that flanges make (and not the Flanges themselves) act as restrictive parameter when we are looking at temperatures. However, the clear limit is 538°C. Above 538°C, you need Carbon content to be more than 0.04%. The moment Carbon %age is more than 0.04, it won't be 304L and you won't be able to claim 304L grade of the dual certified material. However range 425°C - 538°C still remains gray area



   
ReplyQuote
(@shrivallabha)
Estimable Member
Joined: 17 years ago
Posts: 134
 

And some more points have come to light after talking to one experienced material engineer.

In ASME B 31.3 (Process Piping), the allowable values are provided for Pipe as well as fittings upto 1500°F (816°C approx) without any (bar) conditions.

It is NOT just the SS304 behaviour but also the fluid service will have bearing on the temperature restriction. If the fluid is corrosive then at higher temperatures such as 425°C, the material will be susceptible to intergranular corrosion. So you will have to first decide on the fluid properties and then look for restricting temperature range.

Hope this helps.



   
ReplyQuote
(@hvn83)
Eminent Member
Joined: 16 years ago
Posts: 12
Topic starter  

Hi shrivallabha,

Thank you kindly for all your answers, theyve provided much help.

Regards,
Hubert



   
ReplyQuote
Share: