17 years 6 months ago - 17 years 6 months ago #7238 by anbarasan
Piping Materials & Galvanic Corrosion was created by anbarasan
When connecting pipes of various materials their difference in electrode potential may cause galvanic corrosion and serious damage of pipes, valves and other equipment in the system. Under certain circumstances in environments like water with free ions (like salt sea water), acids or bases, higher temperatures and enough oxygen, the systems deteriorate very fast.
A very common connection in piping systems is copper and low-carbon steel. In connections like this steel corrodes many times faster than steel alone.
A metal with lower electrochemical potential will be the cathode in a connection and will remain unchanged. A metal with higher potential will be the anode and will corrode. The list below indicates the galvanic relationship between some materials commonly used in piping systems.
The metals above will resist the metals below. The greater the distance is between two metals, the greater the speed of corrosion
Titanium
Hastelloy C 4)
Monel
Stainless Steel passive
Silver
Bronze
Copper
Brass
Lead-Tin Alloys
Hastelloy A 4)
Stainless Steel 316 1)
Stainless Steel 430 2)
Stainless Steel 410 3)
Cast Iron
Low-carbon Steel
Aluminum Alloys
Magnesium Alloys
1) Austenitic stainless steel with increased molybdenum content to increase resistance to corrosion compared to other 300 series alloys. Resist scaling at temperatures up to 1600oF (871oC). Used in industry, in marine environments and in a wide range of general industrial components.
2) Basic ferritic non-heat treatable stainless steel. Its strengths are in ductility, formability, good corrosion and oxidation resistance, thermal conductivity and finish quality. Used in automotive and architectural trim, heat exchangers and scientific equipment.
3) Martensitic stainless which attain high mechanical properties after heat treatment. Good impact strength, corrosion and scaling resistance up to 1200oF (649oC). Used in cutlery, steam and gas turbine blades and buckets, valve components and fasteners.
4) Hastelloy is a trademark for a series of high-strength, nickel based, corrosion resistant alloys. Other components includes molybdenum and chromium. Hastelloy is used in chemical applications. Resistant to pitting, stress-corrosion cracking and to oxidizing atmospheres up to 1900oF (1037oF).
A very common connection in piping systems is copper and low-carbon steel. In connections like this steel corrodes many times faster than steel alone.
A metal with lower electrochemical potential will be the cathode in a connection and will remain unchanged. A metal with higher potential will be the anode and will corrode. The list below indicates the galvanic relationship between some materials commonly used in piping systems.
The metals above will resist the metals below. The greater the distance is between two metals, the greater the speed of corrosion
Titanium
Hastelloy C 4)
Monel
Stainless Steel passive
Silver
Bronze
Copper
Brass
Lead-Tin Alloys
Hastelloy A 4)
Stainless Steel 316 1)
Stainless Steel 430 2)
Stainless Steel 410 3)
Cast Iron
Low-carbon Steel
Aluminum Alloys
Magnesium Alloys
1) Austenitic stainless steel with increased molybdenum content to increase resistance to corrosion compared to other 300 series alloys. Resist scaling at temperatures up to 1600oF (871oC). Used in industry, in marine environments and in a wide range of general industrial components.
2) Basic ferritic non-heat treatable stainless steel. Its strengths are in ductility, formability, good corrosion and oxidation resistance, thermal conductivity and finish quality. Used in automotive and architectural trim, heat exchangers and scientific equipment.
3) Martensitic stainless which attain high mechanical properties after heat treatment. Good impact strength, corrosion and scaling resistance up to 1200oF (649oC). Used in cutlery, steam and gas turbine blades and buckets, valve components and fasteners.
4) Hastelloy is a trademark for a series of high-strength, nickel based, corrosion resistant alloys. Other components includes molybdenum and chromium. Hastelloy is used in chemical applications. Resistant to pitting, stress-corrosion cracking and to oxidizing atmospheres up to 1900oF (1037oF).
Please Log in or Create an account to join the conversation.
- juan1977
- Offline
- Senior Member
Less More
- Posts: 63
- Thank you received: 0
16 years 2 months ago - 16 years 2 months ago #4501 by juan1977
Replied by juan1977 on topic A very common connection in
A very common connection in piping systems is copper and low-carbon steel.
_________________
I have not seen this type of dissimilar joint in power, refineries and petro chem industries. Ive joined several dissimilar metals in variety of process services by using either a bolted or welded joint - its doable. The AWS has even published a book dealing with this methodlogy. Just need to watch that the environment where its going to start to corrode are avoided.
_________________
I have not seen this type of dissimilar joint in power, refineries and petro chem industries. Ive joined several dissimilar metals in variety of process services by using either a bolted or welded joint - its doable. The AWS has even published a book dealing with this methodlogy. Just need to watch that the environment where its going to start to corrode are avoided.